‌I. Raw material smelting‌
‌Batching and alloy preparation‌

According to the target alloy model (such as 6063, 7000 series), the ratio of aluminum ingots and alloy elements (magnesium, silicon, copper, etc.) is accurately calculated.
The raw materials are put into the smelting furnace, melted to liquid state by natural gas or electric heating, and stirred to ensure uniform composition.
Refining processes (such as rotary degassing and floating slag removal) are used to remove gas and impurities in the aluminum liquid to improve the purity of the material.
‌Casting‌

The refined aluminum liquid is injected into the continuous casting machine and cooled to form cylindrical cast bars (round cast bars), with a diameter range of 80-300mm.
The cast bars need to be homogenized (heated to 500-550℃ for several hours) to eliminate internal stress and improve processing performance.
‌II. Mold design and production‌
‌Mold development‌

According to the requirements of the profile cross-section shape, the mold structure is designed using CAD/SolidWorks software, focusing on key parts such as diverter holes and welding chambers.
The mold is manufactured using high-precision equipment such as CNC milling machines and EDM, and the material is mostly H13 hot-working die steel.
‌Mold processing‌

The mold is vacuum quenched and nitrided to increase the surface hardness (up to 53-54HRC), and polished to a finish below Ra0.4μm.
After the mold test is verified, the die hole size is adjusted by wire cutting to ensure the extrusion molding accuracy.
‌III. Extrusion molding‌
‌Heating and extrusion‌

The cast rod and the mold are heated to 400-500℃ simultaneously, and high pressure (15-50MN) is applied through the extruder to continuously extrude the aluminum from the die hole.
Follow the principle of "high temperature and low speed, low temperature and high speed" to control the extrusion speed (usually 0.5-5m/min) to balance the molding quality and efficiency.
‌Cooling and traction‌

The extruded profile is immediately air-cooled or water-cooled quenched (such as 6063 alloy requires air cooling to achieve T5 state).
The traction machine pulls the profile synchronously and performs preliminary cutting according to the set length (such as 6-6.5 meters).
‌Fourth, post-processing process‌ ‌Straightening and sizing‌ ‌Use a hydraulic straightening machine to adjust the straightness of the profile (error ≤ 0.5mm/m), and cut it to the customer's specified length (±0.2mm accuracy) through a sizing saw.
‌Artificial aging‌ ‌Put the profile into an aging furnace and heat it to 170-200℃, keep it warm for 2-3 hours, and improve the hardness and tensile strength (such as 6063-T6 hardness can reach more than 15HW).
‌Five, surface treatment‌ ‌Pretreatment‌ ‌ ‌Chemical degreasing or alkaline washing to remove surface oil stains, and then acid etching or mechanical polishing to form a clean substrate.
‌Anodizing‌ ‌ ‌Electricity is applied in sulfuric acid electrolyte to generate a 5-25μm aluminum oxide film, and color is given by electrolytic coloring (such as champagne gold, black) or adsorption of dyes.
Sealing treatment seals the micropores of the membrane layer to improve corrosion resistance and wear resistance.
‌Spraying process‌

‌Powder spraying‌: Electrostatically adsorb epoxy resin powder, and after curing, form a 60-80μm coating, with optional matte or glossy effects.
‌Fluorocarbon spraying‌: Use PVDF coating, which has excellent UV resistance and is suitable for outdoor buildings.
‌Sixth, special process for functional profiles‌
‌Broken bridge insulation profiles‌

The inner and outer aluminum profiles are processed into serrated interfaces through a tooth-cutting machine, inserted into PA66 nylon insulation strips, and then pressed by a rolling compound machine to block heat conduction.
The width of the insulation strip is usually 12-34mm, suitable for different energy-saving standards.
‌Wood grain transfer‌

Wood grain transfer paper is covered on the surface of the powder spray substrate, and a three-dimensional imitation wood texture is formed after high-temperature baking, which is used for decorative profiles.