Aluminum Rod Manufacturing Process

May 13, 2025

Leave a message

1. Raw material selection and pretreatment
Alloy grade screening
6 series aluminum alloys (such as 6061, 6063): used for building profiles and automotive structural parts, providing good weldability and medium strength (tensile strength ≥ 310 MPa);
7 series aluminum alloys (such as 7075): suitable for aviation fasteners and high-load components, with ultra-high strength (tensile strength up to 570 MPa);
Impurity control: Fe content needs to be <0.7%, Si content <0.8% to avoid surface cracks during extrusion.
Ingot pretreatment
Homogenization annealing: 480-520℃ insulation for 4-8 hours to eliminate grain boundary segregation and improve extrusion molding stability;
Surface treatment: Mechanical polishing or pickling to remove the oxide layer on the surface of the aluminum rod (Ra≤3.2μm) and reduce the wear rate of the extrusion die.
2. Melting and casting process
Melting parameter control
Temperature control: The melting temperature of non-alloy aluminum is 700-750℃, and the aluminum alloy needs to be reduced to 660-720℃ to prevent the burning of alloy elements;
Refining process: Use argon gas rotation degassing (flow rate 15-20 L/min) to make the hydrogen content ≤0.15 mL/100g Al.
Casting
Deep well casting: Cooling water flow 2-5 m³/h, casting speed 100-150 mm/min, to obtain cast aluminum rods with a diameter of Φ100-500mm; Sawing and sizing: Cast rod cutting length 500-6000mm, end face verticality ≤1°. 3. Core technology of extrusion molding
Mold design specifications
Shunting die structure: used for hollow aluminum bars, the shunt bridge angle is 45-60°, balancing the metal flow rate;
Working belt length: 3-15mm (complex cross-sections need to be designed in sections), and the molding tolerance is controlled to be ±0.1mm.
Process parameter optimization
Alloy type           Extrusion temperature (℃)                 Extrusion speed (m/min)                    Specific pressure (MPa)
6061                   450-480                                              12-25                                                   400-600
7075                   380-420                                              5-10                                                     700-850
Air cooling process: wind speed ≥10 m/s, so that the profile drops from 500℃ to below 200℃ within 60 seconds;
Water mist cooling: water temperature ≤30℃, suitable for thick-walled aluminum bars (wall thickness >10mm).
4. Heat treatment and finishing
Solution treatment (T6 state)
6061 alloy is heated to 530℃±5℃ and kept for 1 hour, and the water quenching cooling rate is >200℃/min;
7075 alloy adopts graded heating: 120℃ preheating → 250℃ medium temperature → 480℃ final temperature.
‌Aging strengthening ‌Natural aging ‌(T4): 96 hours at room temperature, hardness increased to HB 80-90;
Artificial aging ‌(T6): 175℃±5℃ for 8 hours, tensile strength increased by 30%-40%.
‌Precision machining technology ‌CNC turning ‌: spindle speed 2000-3000 rpm, feed rate 0.1-0.3mm/r, surface roughness Ra≤1.6μm;
Cold stretch straightening ‌: elongation 0.5%-3%, elimination of residual stress (accuracy ±0.05mm/m). V. Surface treatment and quality control
Functional surface treatment
Hard anodizing: film thickness 20-50μm, microhardness HV 300-500;
Micro-arc oxidation: breakdown voltage 350-450V, generating ceramic layer (thickness 50-200μm).
‌Testing standards and methods‌
Testing items Instruments and equipment Qualification standards
Composition analysis Direct reading spectrometer (OES) Complies with ASTM B221/EN 754
Mechanical properties Universal testing machine Tensile strength deviation ≤5%
Defect detection X-ray flaw detector Porosity ≤0.5%, no cracks

6.‌Industry technology trends‌
‌Intelligent extrusion‌: Use IoT sensors to monitor mold temperature (accuracy ±1℃) and extrusion pressure fluctuations in real time; ‌Short process manufacturing‌: Continuous casting and rolling process shortens the time from smelting to forming by 40% and reduces energy consumption by 25%; ‌Green surface treatment‌: Chromium-free conversion film technology (coating thickness 1-3μm), compliant with RoHS 3.0 standards. ‌Process Optimization Suggestions‌
For high-precision aviation aluminum bars (such as 7075-T7351), it is recommended to use isothermal extrusion + multi-stage aging process (120℃×6h + 160℃×8h), which can increase fatigue life by 50%;
In the production of aluminum bars for construction (6063-T5), mold nitriding treatment (surface hardness ≥1200HV) can extend the mold life to 800-1000 tons/set.

Aluminum rod manufacturing processaluminum rod manufacturing