8079 Alloy Foil for Battery Applications: Composition and Foil Quality

Sep 01, 2025

Leave a message

Alloy Composition and Why Iron and Silicon Matter

8079 is a low-alloy aluminium foil grade. EN 573-3 specifies 0.7-1.3% Fe and 0.05-0.30% Si, with Cu, Mn, Mg and Ti each held to a maximum of 0.05%, Zn to 0.10%, and other impurities limited to 0.05% each and 0.15% in total. The iron and silicon form fine Al-Fe-Si dispersoids during casting and rolling. Those particles refine the cast grain structure, raise the recrystallisation temperature and increase foil strength, which is exactly what is needed in a product rolled down to 0.006-0.2 mm thickness.

Because the alloy is dilute, the foil keeps high ductility and forms an even, compact natural oxide layer. It is not a high-purity grade, and it does not rely on chromium, nickel or rare-earth additions for its performance.

The EN 546 Foil Specification Framework

EN 546-1 defines the technical conditions for inspection and delivery of aluminium foil, EN 546-2 covers mechanical properties, EN 546-3 covers dimensional tolerances and EN 546-4 covers special requirements such as pinhole limits for critical barrier duties. ASTM B479 is the corresponding specification for annealed aluminium foil for flexible barrier applications, and GB/T 3198 covers aluminium and aluminium alloy foil in the Chinese system. Foil is by definition rolled to a thickness of 0.20 mm or below.

Parameter Typical supply for battery and packaging duty
Thickness 0.006-0.040 mm, most pouch laminates use 20-40 micrometre foil
Width up to 1600 mm slit to customer width, bare or laminated
Temper annealed (O) for lamination and forming
Surface mill finish, low oil residue, uniform brightness
Wettability and pinholes according to EN 546-4 when specified

Function Inside a Pouch Cell

A lithium-ion pouch film is a three-layer laminate: an outer oriented nylon layer for puncture and abrasion resistance, the 8079 or 8021 aluminium foil layer, and an inner cast polypropylene layer that seals against the electrolyte. The aluminium layer performs three jobs - it blocks moisture and gas ingress, it provides the dead-fold behaviour needed to cold-form the pouch pocket, and it carries the mechanical load of the cell during swelling and handling. Foil quality therefore drives two failure modes: pinholes that open a path for moisture, and thickness variation that produces uneven forming and local thinning at the pocket corners.

Quality Control and Delivery

Production control covers chemistry check per heat, tensile and elongation testing per EN 546-2, thickness and width tolerance per EN 546-3, pinhole inspection on a light table, and residual oil measurement. Coils are wound on steel or aluminium cores, wrapped in moisture-barrier film, and supplied with a 3.1 inspection certificate. Foil is stored away from alkaline or acidic vapours because the unprotected surface reacts with strong alkalis and with chloride-bearing atmospheres.

Frequently Asked Questions

Q: What is the difference between 8079 and 8021 foil?
A: Both are Al-Fe-Si foil alloys. 8079 has the higher iron range of 0.7-1.3% and is used where formability and barrier performance are the priorities; 8021 carries a small addition of other elements that raises strength slightly.

Q: Why is the metal layer in a pouch cell kept at 20-40 micrometres?
A: Thinner foil is more prone to pinholes and to failure during deep forming of the pocket; heavier foil adds weight and reduces forming accuracy, so the range is a balance between barrier integrity and cell mass.

Q: Which foil standard should be quoted on a purchase order?
A: EN 546-1 with EN 546-2 mechanical requirements, EN 546-3 tolerances and, where pinhole or wettability limits are needed, EN 546-4.

Q: Can bare 8079 foil be used as a current collector?
A: No. Current collectors are made from higher-conductivity 1xxx series foil; 8079 is specified as the packaging barrier layer of the pouch laminate.

Q: How is foil quality verified before lamination?
A: By chemistry and mechanical tests to EN 546-2, dimensional checks to EN 546-3, light-table pinhole inspection and residual oil measurement on samples taken from each coil.