What 3004 and 3104 Are
3004 and 3104 are aluminium alloys of the 3xxx family built on a manganese base with a deliberate magnesium addition, which is why they are often described as Al-Mn-Mg rather than simply Al-Mn. Manganese provides solid-solution strengthening and improves the strain-hardening response, while magnesium adds further strength and raises resistance to attack in water and in industrial atmospheres. Both grades remain non-heat-treatable: their properties come from cold reduction and from the annealing or stabilising treatment applied afterwards.
The two grades are close relatives. 3104 is a tighter-controlled variant developed for container stock, with composition and microstructure balanced so that thin-gauge bodies and ends can be drawn and necked at high line speeds without tearing. 3004 is the more general-purpose grade, widely used in roofing, siding, transport panels and general sheet-metal work.
Temper Designations Explained
Temper letters and digits are defined by the four-digit system harmonised in ANSI H35.1. The letter H means strain hardened. The first digit gives the treatment sequence, and the second digit gives the strength level, where 2 is quarter hard, 4 is half hard, 6 is three-quarter hard and 8 full hard.
| Temper | Treatment | Strength level | Relative strength within 3004/3104 |
|---|---|---|---|
| H16 | Strain hardened only | Three-quarter hard | Below H18 |
| H18 | Strain hardened only | Full hard | The hardest of the four |
| H22 | Strain hardened and partially annealed | Quarter hard | Between H24 and O |
| H24 | Strain hardened and partially annealed | Half hard | Above H22, below H16 |
The important point is that H1x and H2x tempers are not points on one continuous scale. H18, for instance, does not sit above H24 because the number is larger; H18 is a fully hard temper while H24 is only half hard, so H18 is distinctly stronger and much less formable. The H2x series exists because partial annealing after cold work restores ductility and removes the risk of delayed ageing and Luder banding that unstabilised H1x material can show, which is why H24 rather than H18 is specified for parts that must be bent after forming. Within a single series the sequence is monotonic: H22 is softer than H24, and H24 is softer than H26.
Mechanical Behaviour and Formability
The precise minima for tensile strength, yield strength and elongation for each temper are tabulated in ASTM B209, and those tables, not general descriptions, should be used for design. As a working rule, moving from H22 through H24 and H16 to H18 raises strength while lowering elongation and increasing the minimum bend radius needed to avoid cracking. For a canopy panel that will be roll-formed, H24 or H26 is usually chosen; for a container body that must resist internal pressure at thin gauge, H19 or H18 drawing stock is used. Because the alloys are not precipitation hardened, welded joints in the heat-affected zone lose only the work-hardening contribution, and property recovery after welding is limited by the fact that no ageing treatment is available.
Typical Applications
Beverage cans and ends. 3104 in the hardest tempers is standard for drawn and ironed bodies and for easy-open end stock, where thin gauge and high strength must combine with extreme formability.
Roofing and wall cladding. 3004 in H24, H26 or H34 type tempers offers weathering resistance and enough strength to span purlins without oil-canning.
Transport panels. Truck bodies, trailer skins, bus panels and rail interior linings use 3004 where a combination of stiffness, low weight and corrosion resistance is needed.
General sheet metal. Enclosures, ducts, tanks and fabricated components that will be bent or rolled after delivery.
Packaging and closures. Foil stock, capsules and container components made from thin 3004 and 3104 gauges.
Processing and Fabrication Notes
Bending is the operation that most often decides the temper. With the softer H22 and H24 conditions a bend radius of about one material thickness is usually achievable, whereas H16 and H18 need noticeably larger radii or a pre-anneal at the bend line. Forming across the rolling direction is preferred because surface roughening, sometimes called orange peel, is more likely when bending along the rolling direction in hard tempers.
Welding is straightforward with the 4xxx and 5xxx filler metals; 4043 is the usual choice for general fabrication. Heat input should be kept moderate to limit distortion, and the weld area must be cleaned of oxide immediately beforehand. Where the finished part will be anodised, welded joints should be dressed and the anodising quality checked, since manganese and magnesium in the weld and heat-affected zone colour differently from the parent metal. For roofing and cladding, cut edges should be deburred and, on exposed external faces, edge-sealed or coated to prevent staining.
Common Misconceptions
"H18 and H24 are steps on one strength ladder." They are not; H18 is full hard while H24 is half hard, and H24 is the weaker and more formable of the two.
"Higher temper number means better quality." It means harder metal with lower elongation, which is often wrong for a component that has to be formed.
"3004 is simply 3003 with more manganese." The magnesium addition changes the strengthening and corrosion behaviour, not only the strength level.
"These alloys can be age hardened after welding." They are non-heat-treatable, so no post-weld ageing treatment exists.
"Can stock and roofing stock are interchangeable." 3104 container stock is produced to tighter gauge and cleanliness limits than general 3004 sheet and is not a like-for-like substitute.
FAQ
Q: Which is stronger, H18 or H24?
H18 is stronger; it is a fully hard strain-hardened temper, while H24 is strain hardened and then partially annealed to the half-hard level.
Q: Why specify H24 instead of H18 for bent parts?
Partial annealing restores ductility, so H24 forms without cracking and does not develop the strain marks that hard tempers can show.
Q: What is the difference between 3004 and 3104?
3104 is a closely controlled container-grade variant with tighter composition and cleanliness requirements; 3004 is the general-purpose version of the same family.
Q: Can 3004 be anodised?
It can, but the manganese and magnesium content produce a darker, satin film, so the process is used for functional protection rather than bright decorative finishes.
Q: Is 3004 suitable for marine use?
It resists fresh water and normal weathering well, but grades such as 5052 and 5083 with higher magnesium content are preferred for sustained salt-water exposure.
Q: Do these alloys need post-weld heat treatment?
No; since they are non-heat-treatable, strength is governed by cold work and no ageing treatment applies after welding.