1050 H22 Anodized Aluminum Coil, 99.5% Al, ASTM B209 Coil Stock

Jan 14, 2026

Leave a message

The 1050 Base Alloy

1050 is a 1000-series aluminium with a minimum aluminium content of 99.5%, which makes it the purest grade in normal commercial use for coil anodising. Only iron and silicon are present in meaningful quantity, at about 0.45% combined, and both are controlled because they form second-phase particles that can roughen an anodic film. The low level of alloying elements gives high electrical and thermal conductivity, excellent reflectivity and very consistent forming behaviour.

The grade cannot be strengthened by heat treatment. Every increase in strength comes from cold reduction, and every softening step comes from annealing, so the temper designation is simply a record of how much cold work the coil retains when it leaves the mill.

What H22 Means

Under the four-digit temper system of ANSI H35.1, the letter H marks a strain-hardened product and the first digit describes the treatment that follows the cold work. H2x means the material was strain hardened and then partially annealed, which raises ductility and removes part of the internal stress without returning the metal to the fully soft O condition. The second digit gives the strength level, and 2 stands for quarter hard. A 1050 H22 coil therefore sits at roughly quarter-hard strength but with better residual elongation than a 1050 H12 coil of the same gauge, which is exactly the combination that coil anodising lines need.

Temper Treatment Relative strength Typical use
O Annealed Lowest Deep forming, bonding
H22 Strain hardened and partially annealed Quarter hard Anodised coil, formed panels
H24 Strain hardened and partially annealed Half hard Stiffer flat panels
H32 Strain hardened and stabilised Quarter hard 5052 panels, marine trim

How the Anodic Film Is Built

Anodising is an electrochemical conversion process. The coil or panel is made the anode in a dilute sulphuric acid electrolyte, typically at 15 to 20 degrees Celsius, and the applied current grows an aluminium oxide film from the substrate itself. The film is porous: it consists of a thin compact barrier layer at the metal interface covered by a honeycomb of cells roughly 10 to 30 nanometres across, and those pores are what make colouring possible.

Film thickness Typical service
5 to 10 micrometres Interior decorative coil, printed and dyed finishes
10 to 15 micrometres Interior architectural trim, appliance and lighting parts
18 to 25 micrometres Exterior architectural use and abrasion-exposed surfaces

Colour is introduced in one of three ways. Organic dyes are absorbed into the pores and give the widest colour range for interior work. Electrolytic colouring deposits inorganic pigments at the base of the pores and produces the bronze and black tones that hold up best outdoors. Integral colour anodising uses modified electrolytes to grow a self-coloured film with excellent light fastness. Whichever route is used, the pores must then be sealed, normally by boiling deionised water or by a cold nickel-fluoride seal, which converts the pore walls to hydrous oxide and locks the colour in.

Coil Anodising versus Sheet Anodising

Continuous coil anodising passes a long web through the process tanks and produces a uniform film along tens or hundreds of metres of material. That consistency is hard to match with rack anodising of cut sheets, where contact marks, edge effects and variation between racks are common. Coil processing also lets a converter supply pre-anodised stock that can be slit, formed and bent afterwards, so long as the forming radius is generous enough not to craze the film.

Applications

Lighting. Luminaire reflectors and bodies take advantage of the whiteness, reflectivity and non-yellowing nature of an anodised 1050 surface.

Nameplates and trim. Dye-coloured coil is used for machine faceplates, badges and decorative strips that need a hard, printable surface.

Interior architecture. Ceiling panels, column covers and lift interiors in clear or bronze finishes.

Appliance and consumer goods. Panels and housings where a scratch-resistant, non-painted finish is preferred.

Housings and enclosures. Electronic and instrument cases that need a durable, electrically insulating outer layer.

Processing Notes

Forming should be carried out across the rolling direction where possible, and bend radii should be increased relative to bare metal because a 10 to 20 micrometre oxide film is brittle in tension. Laser cutting is preferred over shearing for visible parts, since shear burrs break the film edge and can start filiform corrosion. When anodised parts must be welded, the film has to be removed locally and the weld re-anodised separately, because welding destroys the oxide in the heat-affected zone. Cleaning should use neutral or mildly alkaline products; strong alkalis attack the film, and abrasive pads leave a permanently visible mark.

Common Misconceptions

"H22 is a heat treatment." It is a cold-work plus partial-anneal condition; 1050 never responds to heat treatment.

"Anodising makes the part much stronger." The oxide layer is hard and abrasion resistant, but it is microns thick and does not raise the load capacity of the coil.

"All alloys anodise to the same colour." 1050 gives a clear, bright film, while 3003 is slightly satin and 5052 distinctly grey because of its alloying elements.

"Anodising is a coating that can peel." The film is grown from the substrate and is integral to it, so it cannot flake off in the way paint can.

"A sealed surface needs no care." Sealing closes the pores but does not make the surface immune to strong alkali or to scratching by hard abrasives.

FAQ

Q: What is the difference between H22 and H24?
Both are strain hardened and partially annealed, but H24 is the half-hard level and H22 the quarter-hard level, so H22 is softer and easier to form.

Q: Can 1050 H22 coil be bent after anodising?
Yes, within limits; the bend radius should be larger than for bare metal because the anodic film is brittle and craze marks appear on tight bends.

Q: Which anodising thickness suits outdoor use?
Exterior exposure normally calls for about 18 to 25 micrometres with electrolytic colouring and a proper seal.

Q: Why does anodised 1050 look brighter than anodised 5052?
Because 1050 contains almost no alloying elements, its film is clear and colourless, while magnesium in 5052 darkens the film.

Q: Is the anodic film electrically conductive?
No; aluminium oxide is a dielectric, so anodised surfaces must be masked or locally stripped wherever an electrical bond is required.

Q: How should anodised coil be stored?
In a dry, ventilated area away from alkalis and abrasive dust, with sheets interleaved or protected so that faces do not rub in transit.